Advances in Preparation and Applications of Disentangled Ultrahigh Molecular Weight Polyethylene - In non-metallocene sy
Ning et al. successfully developed a series of β-diketonate titanium(IV)/diethylaluminum chloride catalytic systems [61]. This is the first report of such catalytic systems for the one-reactor synthesis of bimodal polyethylene (polyethylene wax PEW/UHMWPE) and d-UHMWPE. By regulating the polymerization conditions and the catalyst structure, the content of the PEW component in the product can be ef
In non-metallocene systems, Ivancheva et al. systematically investigated the self-immobilizing polymerization behavior of phenoxyimine titanium complexes bearing allyloxy functional groups [55-58]. They found that after introducing allyloxy groups into the catalyst structure, the polymerization kinetics exhibited a distinct two-stage character: an initial rapid homogeneous polymerization phase, followed by a transition to a constant-rate heterogeneous polymerization phase induced by catalyst self-immobilization. Through infrared spectroscopy analysis, characteristic absorption peaks of the phenoxy group were detected in the resulting polyethylene, whereas no such signal was observed when using a control catalyst without allyloxy groups, directly confirming that the catalyst was incorporated into the polyethylene chain through copolymerization. The degree of self-immobilization is significantly influenced by the ligand structure: when the phenoxy group contains a medium-sized substituent, the self-immobilization rate is highest, with approximately 80% of the catalyst being immobilized within a few minutes; in contrast, tert-butyl or large substituents hinder rapid self-immobilization. The resulting polyethylene has an extremely high molecular weight, with a number-average molecular weight ranging from 2.0 × 106 to 7.0 × 106 g/mol, and contains almost no methyl or vinyl end groups, indicating a highly linear structure. More importantly, the particle morphology of the polyethylene powder prepared using the self-immobilizing catalyst has been significantly improved; the particles are nearly spherical and do not adhere to the reactor walls, effectively resolving the engineering challenges associated with homogeneous polymerization.
Two representative architectures of self-immobilizing FI catalysts are compared in Figure 4. Oleynik et al. further expanded the structural scope of self-immobilizing FI catalysts, synthesizing phenoxyimine titanium complexes bearing diallylamino substituents, with the allyl group located at the meta or para position of the N-aryl ring (Figure 4b) [59]. The study showed that the introduction of the diallylamino group not only confers self-immobilizing capability on the catalyst but also stabilizes the active center through its strong electron-donating effect, suppressing β-hydrogen transfer. Under optimized conditions (Al/Ti = 500, 40°C, 0.4 MPa ethylene), the polymerization activity reached as high as 14.0 × 106 g PE/(molTi·MPa·h), and the resulting polyethylene had a molecular weight of up to 4.1 × 106 g/mol, a melting point as high as 143.7°C, and a crystallinity exceeding 85%. Compared with allyloxy analogues, the diallylamino system exhibits higher crystallinity and superior particle morphology. Annealing experiments showed that, as the annealing time increased, the area under the low-temperature melting peak on the DSC curve gradually increased, while the area under the high-temperature peak correspondingly decreased, a characteristic typical of nascent, disentangled UHMWPE.
Wang et al. approached FI catalyst functionalization from a different perspective [60]. They synthesized phenoxyimine titanium complexes bearing ethylphenyl or vinylphenyl substituents at the para position of the N-aryl group. Single crystal X-ray diffraction revealed that the titanium center adopted a distorted octahedral geometry with cis-N, trans-O, cis-Cl coordination mode. Upon activation with dry MAO, these catalysts exhibited good polymerization activity under mild conditions (room temperature, ethylene pressure 0.1 MPa), and the molecular weight of the polyethylene could be controlled to ultrahigh levels (Mw > 1.0 × 106 g/mol) simply by varying the polymerization time. It is worth noting that when using complexes containing vinylphenyl groups, an increase in polymerization time may lead to a decrease in molecular weight, suggesting that chain-transfer reactions gradually become predominant. This indicates that the position and reactivity of terminal double bonds have a significant impact on the “pseudoactive” behavior of the catalyst. Nevertheless, this class of catalysts offers a new approach for the preparation of UHMWPE under mild conditions via a simple process.
Ivanchev et al. further evaluated the practical performance of self-immobilizing phenoxyimine catalysts with different structures in the preparation of UHMWPE reactor powders [58]. One of these structures is shown in Figure 4a. The results showed that the complex bearing cumyl substituents produced UHMWPE with a crystallinity as high as 80% and a number-average molecular weight of 2.6 × 106 g/mol. After solid-state processing, the product exhibited a tensile modulus of 136 GPa, a tensile strength of 2.66 GPa, and an elongation of 3.1%. Although these values were slightly lower than those of the non-self-immobilizing reference system, the reactor fouling phenomenon was greatly alleviated. Catalysts III (phenoxy with a methyl group at the para position) and IV (containing a methoxy group) exhibited slightly lower mechanical strength. Overall, the self-immobilizing strategy significantly improved the stability of the polymerization process and the morphology of the powder particles at the cost of a slight reduction in mechanical properties, providing a viable approach for the industrial production of d-UHMWPE.
In summary, self-immobilizing catalysts achieve a spontaneous transition from homogeneous to heterogeneous catalysis through the clever design of polymerizable functional groups in the ligand. While maintaining the excellent performance of single-site catalysts, they overcome the inherent engineering drawbacks of homogeneous polymerization and can produce UHMWPE with low entanglement characteristics at relatively high polymerization temperatures. This strategy represents one of the most promising directions for the industrialization of disentangled UHMWPE.
2.3 Supported Multi-Active-Center Catalysts
Smith et al. supported a VCl3 catalyst on a glass slide and successfully prepared UHMWPE films with different entanglement densities over a wide temperature range (−40°C to 90°C) by varying the polymerization temperature [15]. The lower the polymerization temperature, the lower the chain entanglement density, and the films exhibited good drawability below the melting point, enabling direct drawing into high-strength, high-modulus fibers. However, the activity of the VCl3 catalyst at low temperature is extremely low, making industrialization unfeasible.
Ning et al. successfully developed a series of β-diketonate titanium(IV)/diethylaluminum chloride catalytic systems [61]. This is the first report of such catalytic systems for the one-reactor synthesis of bimodal polyethylene (polyethylene wax PEW/UHMWPE) and d-UHMWPE. By regulating the polymerization conditions and the catalyst structure, the content of the PEW component in the product can be effectively controlled in the range of 2%–60%. The catalytic system achieved optimal activity under low-temperature (0°C) polymerization conditions, at which point the PEW content in the product was below 5%. After extracting and separating PEW, the disentangled state of the UHMWPE component was confirmed by melt rheological testing, thermal analysis, and solid-state NMR characterization. d-UHMWPE synthesized at 0°C can be processed via solvent-free solid-state processing and exhibits excellent tensile properties, with a tensile strength exceeding 800 MPa and a modulus of elasticity exceeding 56 GPa. β-diketonate titanium complexes can be prepared using a single-pot, one-step method. The study suggests that the multiple active centers in this catalytic system originate from its heterogeneous composition. Their formation mechanism is related to ligand dynamics, the equilibrium between mononuclear and binuclear structures, and the coexistence of multiple complexes, and is not affected by the ligand-to-metal stoichiometric ratio.
In addition to lowering the polymerization temperature to reduce the entanglement degree, increasing the distance between active sites is another effective strategy for preparing d-UHMWPE.
Chammingkwan, Bando, et al. applied a MgO/MgCl2/TiCl4 core-shell catalyst to the synthesis of UHMWPE [62]. The catalyst is simply prepared by reacting MgO nanoparticles with TiCl4, which forms a thin layer of MgCl2 on the surface and anchors TiCl4. Since MgO is a non-porous material, the polymerization activity shows a good linear relationship with the specific surface area. However, unmodified MgO disperses extremely poorly in non-polar solvents, leading to severe catalyst agglomeration and the formation of blocky, coarse polymer morphology. Through modification with methyl oleate (MO), the carboxylate groups formed bridging coordination with Mg atoms, effectively suppressing agglomeration. The MO-modified catalyst successfully produced dispersed UHMWPE particles ranging from 100 to 200 μm in size, with an activity as high as 8670 g PE/g Cat and a molecular weight of 3.0 × 106 g/mol, laying the foundation for subsequent studies on micronization and reduced entanglement.
Further screening of surface modifiers revealed that polyoxyethylene alkylamine (PA), due to its multiple anchoring sites, can form a stable adsorption layer on the MgO surface, achieving true primary particle dispersion of the catalyst in heptane (D50 = 0.07 μm). This nano-dispersed catalyst, when used for polymerization at 70°C, directly produced ultrafine UHMWPE particles with a size of 1–2 μm, which is in excellent agreement with theoretical calculations. These ultrafine powders can significantly reduce the melting temperature during compression molding by 20°C, indicating that the minute voids between ultrafine particles and the larger contact interface promote inter-particle sintering [63].
Chammingkwan et al. subsequently elucidated the intrinsic mechanism by which this type of catalyst produces d-UHMWPE [64]. Since the catalyst consists of non-porous single particles, the polymer chains can crystallize immediately after growing from the surface, avoiding the aggravated chain entanglement caused by pore confinement in porous supports and the localized melting induced by polymerization heat. DSC annealing experiments showed that the melt-recrystallization peak area fraction of UHMWPE prepared with the nano-dispersed catalyst increased significantly with annealing time, whereas that of commercial UHMWPE remained almost unchanged, indicating a low initial entanglement density. Furthermore, by adding butylated hydroxytoluene (BHT) to the cocatalyst to increase the ligand volume, the density of effective active sites was reduced, extending the characteristic relaxation time from 2731 to 4373 s and further decreasing the entanglement density. This work demonstrates that the nano-dispersed MgO/MgCl2/TiCl4 catalyst can directly synthesize d-UHMWPE at industrial polymerization temperatures through two mechanisms: “non-porous surface crystallization” and “regulation of active site density.” A schematic diagram is shown in Figure 5. In Figure 5a, poreless and nano-dispersed features allow the growing chains to crystallize without disturbance of other chains confined in pores [64]. The illustration in gray represents the active sites on primary building units of a typical Ziegler–Natta catalyst. In Figure 5b, reducing the active-site density with bulky alkylaluminum increases the distance between the active sites to promote the formation of more weakly entangled polymer [64].
The research group of Li reported a series of POSS-barrier-supported Z–N catalysts for the preparation of disentangled UHMWPE [65, 66]. Due to the strong electron-withdrawing effect of the dihydroxy groups in POSS molecules, they exhibit higher binding energy with Mg 2p and Ti(IV) 2p orbitals, enabling the capture of MgCl2 and TiCl4 to form nano-aggregates [65]. These aggregates are uniformly distributed on the silica gel surface, with sizes much larger than the folding length of polyethylene chains (approximately 20–30 nm), and can effectively isolate adjacent active sites and growing polymer chains. A schematic diagram is shown in Figure 5c. In the figure, “a” represents polymerization time, “b” represents cocatalyst dosage, “c” represents POSS loading, and “d” represents temperature. DFT calculations and XPS results indicate that the dihydroxyl groups in POSS form a stable coordination structure with MgCl2, enhancing the electron-deficient character of Mg and Ti, thereby reducing the catalytic activity of the nanoaggregates. The authors refer to this as a “horizontal isolator,” which has extremely low activity on its own but effectively prevents interchain overlap. More importantly, this study used rheological methods to characterize the entanglement density of the primary chains in UHMWPE based on the initial storage modulus G′t=0. The results show that the entanglement density decreases exponentially as the POSS content increases. In addition, the study revealed a relationship between entanglement density and polymerization activity: at a constant temperature, entanglement density increases linearly with activity; whereas under elevated-temperature conditions, entanglement density increases as a power function. The isolation effect of POSS/MgCl2 nanoaggregates counteracts the tendency for entanglement to form rapidly at high temperatures, thereby enabling the preparation of UHMWPE with low entanglement at industrial temperatures of 60°C–85°C, with an activity of 2700 kg PE/(molTi·h). Subsequently, the research team chemically anchored POSS molecules onto the surface of triethylaluminum (TEA)-treated silica gel, successfully developing a novel POSS-modified Z–N catalyst [66]. Studies have shown that POSS molecules are dispersed at the molecular level on the silica gel surface, without self-aggregation or crystallization. The residual silanol groups (≡SiOH) on POSS can capture Mg/Ti compounds through protonation, forming a vertical support structure that “elevates” the active sites away from the silica surface. This structure significantly reduces the heterogeneity of the active sites, resulting in exclusively tetra-coordinated Mg2+ sites, rather than the mixed tetra-coordinated and penta-coordinated states found in conventional catalysts. Using techniques such as CO probe infrared spectroscopy (CO-DRIFT), XPS, and ultraviolet–visible (UV–vis) spectroscopy, it was confirmed that POSS modification enhanced the Lewis acidity of the active sites and resulted in a more uniform coordination environment. Ultimately, the molecular weight distribution of the UHMWPE produced by ethylene polymerization using this catalyst decreased from 6.7 to 3.9, while maintaining high catalytic activity.
2.4 Comparison of the Catalyst Families
In summary, the three families of catalysts are not equally effective in reducing the entanglement density of the nascent powder. Homogeneous single-site catalysts are the most effective because their active centers are inherently isolated; they operate, however, only at low temperature, at which crystallization is faster than chain propagation, which makes industrial implementation difficult. Supported single-site catalysts preserve this low-entanglement advantage as far as possible while also providing a good particle morphology and moderate reaction conditions. Modified heterogeneous catalysts, by contrast, are the only route that operates at industrially relevant temperatures, although their entanglement density is higher than that of the single-site catalysts.
3 Key Characterization Techniques for Disentangled UHMWPE
The entanglement state of nascent UHMWPE powder can be characterized through rheological and thermodynamic methods, both of which are based on differences in melting behavior caused by different entanglement states [5, 25, 67]. Among these, rheology is the most mature method for characterizing polymer entanglement states, while thermodynamic low-temperature annealing can qualitatively characterize the entanglement state of UHMWPE. In solid-state stretching experiments, a higher draw ratio also implies a lower entanglement density and can be used for qualitative analysis [68]. It should be noted, however, that the draw ratio is not the most reliable indicator of the entanglement state. Strain hardening is a better indicator. Bartczak showed this by plane-strain compression, in which the deformation remains homogeneous up to high strains—unlike in a tensile test. When the entanglement density of the amorphous phase is lowered, the strain hardening modulus decreases and strain hardening begins at higher strain; when it is raised, the network becomes stiffer and strain hardening starts earlier [69]. Both quantities therefore change systematically with the entanglement density, which makes them a sounder measure than a single draw ratio value. In the following sections the draw ratio is still used as the working descriptor, simply because almost all of the publications reviewed here report it, whereas strain hardening data exist for only a few systems; this allows the results of the cited works to be compared on a common basis. These values should nevertheless be read as a qualitative indication of the entanglement state. X-ray diffraction and scattering can characterize crystalline information, and solid-state nuclear magnetic resonance (NMR) can characterize the mobility of molecular chains and the amorphous region structure, serving as auxiliary characterization methods for the entanglement state of nascent UHMWPE powder [8, 42, 47, 70-72].
3.1 Rheological Characterization
原文出处:https://onlinelibrary.wiley.com/doi/10.1002/app.71693#3
提示:本站仅汇集公开信息,版权归原作者与原发布媒体所有。
提示:本站仅汇集公开信息,版权归原作者与原发布媒体所有。